Brass Grade

FREE CUTTING BRASS RODS - GRADE I

IS 319 / 89 NR. EQUIVALENT SPEC. BS 2874 / 86, CZ121PB3,JIS3250H C-3604, ASTMBC38500

Chemical Requirements (%) Grade I
Copper
56.0 – 59.0 %
Lead
2.0 – 3.50 %
Iron
0.35% max.
Total Imp. Excl. Iron
0.70% max.
Zinc Remainder
Physical Properties
Condition Size T. S. MPA EL % Min

Annealed (O)

6-25 345 12
25-50 315 17
50 above 285 22
Half-Hard (HB) 6-12 405 4
12-25 395 6
25-50 355 12
Hard (HD) 50 above 325 17
6-12 550
12-25 490 4
Fabrication Properties  
Capacity for being
 
Cold worked
Poor
Hot formed
Fair
Machinability Rating
100%
Suitability for Soldering
Excellent
Suitability for Brazing Good

FREE CUTTING BRASS RODS - GRADE Il & lll

IS 319 / 89 NR. EQUIVALENT SPEC. BS 2874 / 86 CZ124, JIS3250 H C-3602, ASTMBC36000

Chemical Requirements (%)Grade IIGrade III
Copper60.0 – 63.0 %60.0 – 63.0 %
Lead2.50 – 3.70 %0.50 – 1.50 %
Iron0.35 % max.0.20 % max.
Total Imp. Excl. Iron0.50 % max.0.50 % max.
ZincRemainderRemainder
Physical Properties Grade II Grade III
Condition Size T. S. MPA EL % Min T. S. MPA EL % Min

Annealed (O)

6-25 355 15 315 22
25-50 305 20 285 27
50 above 275 25 255 32
Half-Hard (HB) 6-12 395 7 355 8
12-25 385 10 345 12
25-50 345 15 305 22
Hard (HD) 50 above 315 20 285 27
6-12 550 460
12-25 485 4 400 4
Physical Properties Grade II Grade III
Capacity for being  
Cold workedPoorFair
Hot formedFairExcellent
Machinability Rating90%80%
Suitability for SolderingExcellentExcellent
Suitability for BrazingGoodExcellent

FREE CUTTING BRASS RODS WITH IMPROVED DUCTILITY

BS 2874 – CZ 131 NR, EQUIVALENT SPEC. DTD 627, EN CW606N – 12164
DIN CuZn36Pb2 – 17900, UNS – C35300

Chemical Requirements(%)
Copper 61.00 – 63.00 %
Lead 1.50 – 2.50 %
Iron – 0.20 % max
Total Imp Excl. Iron – 0.50 % max
Zinc Remainder
Physical Properties : (1/2 Hard)
Condition Size T. S. MPa EL % Min.
Half-Hard (AB) 6 – 18 350 22
  18 – 40 350 25
  40 – 80 350 28
  Above 80 mm 330 28
Fabrication Properties
Capacity for being  
Cold Worked Poor
Machinability Rating (IS 319-I 100) 70
Bending Excellent
Cold Heading Excellent
Rivetting Excellent

FREE CUTTING & FORGING BRASS RODS

EN 12164 : 1998

  A B
Chemical
Requirement(%)
CuZn39Pb3 CuZn40Pb2
CW614N CW617N
Copper 57 – 59 % 57-59 %
Lead 2.5 – 3.5 % 1.6 – 2.5 %
Aluminum 0.05 % max 0.05 % max
Iron 0.30 % max 0.30 % max
Nickle 0.30 % max 0.30 % max
Tin 0.30 % max 0.30 % max
Total Imp. 0.20 % max 0.20 % max
Zinc Remainder Remainder
Physical Properties : (1/2 Hard)
Condition Size T. S. MPa EL % Min. Size T. S. MPa EL % Min.
Half-Hard (AB) 6 -14 400 15 6 -14 550  
  14 – 40 380 18 14 – 40 500 8
  40 – 80 360 20 40 – 80 430 10
Fabrication Properties
Capacity for being 
Cold WorkedPoor
Hot FormedExcellent
Suitability for SolderingExcellent
Suitability for BrazingGood

FORGING BRASS RODS

BS 218

Chemical Requirement (%)
Copper56.50 – 60.00 %
Lead1.00 – 2.50 %
Iron0.30 % max
Total Imp.0.70 % max
ZincRemainder
Physical Properties
Rm – Tensile strength in Kg / mm2 32 min.
Elongation on 5.65 A% 25 min.
Fabrication Properties
Capacity for being
 
Cold Worked Poor
Hot Formed Excellent
Hot Forgebility Rating (Forging Brass – 100 ) 100
Machinability Rating (IS 319-I 100) 80
Suitability for Soldering Excellent
Suitability for Brazing Good

FORGING BRASS RODS

IS – 6912 / 2005 FLB

Chemical Requirement (%)
Copper 56.50 – 60.00 %
Lead 0.60 – 2.00 %
Iron 0.30 % max.
Total Imp excl Fe 0.75 % max
Zinc Remainder
Physical Properties
Rm – Tensile strength in Mpa 310 min.
Elongation on 5.65 A% 25 min.
Fabrication Properties
Capacity for being
 
Cold Worked Poor
Hot Formed Excellent
Hot Forgebility Rating (Forging Brass – 100 ) 100
Machinability Rating (IS 319-I 100) 80
Suitability for Soldering Excellent
Suitability for Brazing Good

FORGING BRASS RODS

IS 3488 / 80 NR. EQUIVALENT SPEC. BS 2874 / 86 CZ122,ASTMBC37700

Chemical Requirements (%) CuZn42Pb2 CuZn40Pb2
Copper 56.5 – 60.0 % 57.0 – 59.0 %
Lead 0.60 – 2.0 % 1.50 – 2.50 %
Iron 0.30 % max. 0.40 % max.
Total Imp. Excl. Iron 0.20% max 0.70 % max
Zinc Remainder Remainder
Physical Properties
Tensile Strength 380 Mpa Min 40 kg/mm2 min
Elongation % 25% Min 18% Min.
Izod Value 2.0 KJ Min.
Fabrication Properties
Capacity for being    
Cold worked Poor Poor
Hot formed Excellent Excellent
Hot forgeability Rating 100% 100%
Machinability Rating 80% 80%
Suitability for Soldering Excellent Excellent
Suitability for Brazing Good Good

SPECIAL FORGING BRASS RODS FOR VALVES

IS 8737 / AMD – 2

Chemical Requirements %
Copper 56.5 – 60.0 %
Lead 1.0 – 2.0 %
Manganese 0.50 % max.
Iron 0.30 % max.
Total Imp. 0.75% max.
Zinc Remainder
Physical Properties
Tensile Strength 40 kg/mm2 Min
Elongation % 18% Min.
Izod Value 2.2 Kgf Min.
Fabrication Properties
Capacity for being  
Cold worked Poor
Hot formed Excellent
Hot forgeability Rating 100%
Machinability Rating 80%
Suitability for Soldering Excellent
Suitability for Brazing Good

RIVETING QUALITY BRASS RODS & WIRES

IS 4170 / 67 NR. EQUIVALENT SPEC. BS 2874 / 86 CZ 109,
JIS3250H C-2800, ASTMBC36500

Chemical Requirements % CuZn40
Copper 59.0 – 62.0 %
Lead 0.75 % max.
Iron 0.10% max.
Total Imp. Excl. Iron 0.30 % max.
Zinc Remainder
Physical Properties
Tensile Strength 40 kg/mm2 Min
Elongation % 18% Min.
Izod Value 2.2 Kgf Min.
Fabrication Properties
Capacity for being  
Machinability Rating 55 %
Bending Excellent
Riveting Excellent
Forging Excellent

RIVETING QUALITY BRASS RODS (LEAD FREE)

IS 4413 / 81 NR. EQUIVALENT SPEC. BS 2872 / 86 CZ 108

Chemical Requirements % CuZn37 CuZn30
Copper 62.0 – 65.0 % 60.5 – 71.50 %
Lead 0.30 % max. 0.05 % max.
Iron 0.10 % max. 0.05 % max.
Total Imp. 0.60 % max. 0.30 % max.
Zinc Remainder Remainder
Physical Properties
Condition T. S. MPa EL % Min T. S. MPa EL % Min
Annealed (O) 325 min 35 % 315 min 45 %
Half-Hard (HB) 460-620 460-620
Hard (HD) 660-775 620 min
Fabrication Properties
Capacity for being  
Machinability Rating 40 %
Bending Excellent
Riveting Excellent
Forging Excellent

RIVETING BRASS RODS (LEADED)

IS 2704 / 83 NR. EQUIVALENT SPEC. BS 2874 CZ 119
JIS3250 H C-2700, ASTMBC34000

Chemical Requirements % CuZn35Pb1 CuZn35
Copper 62.0 – 65.0 % 63.0 – 68.0 %
Lead 0.75 – 1.50 % 0.02 % max.
Iron 0.10 % max. 0.05 % max.
Total Imp. 0.50 % max. 0.30 % max.
Zinc Remainder Remainder
Physical Properties
Condition T. S. MPa EL % Min T. S. MPa EL % Min
Quarter Hard (HA) 325-390 30% 340-345 30%
Half-Hard (HB) 400-490 20% 420-510 15%
Hard (HD) 500-685 15%
Extra Hard (HE) 695-885 5%
Fabrication Properties
Capacity for being  
Cold Forming Excellent
Machinability Rating 70 %
Bending Excellent
Riveting Excellent

HIGH TENSILE BRASS RODS

IS 320 / 80 NR. EQUIVALENT SPEC. BS 2874 CZ 114 & CZ 115,
JIS3250H C6782 & C6783

Chemical Requirements % HT1 HT2
Copper 56.0 – 60.0 % 56.0 – 61.0 %
Lead 0.20 – 1.50 % 0.50 – 1.50 %
Iron 0.20 – 1.25 % 0.20 – 1.50 %
Tin 0.20 – 1.0 % 1.0 % max
Aluminum 0.20 % max. 0.30 – 2.0 %
Manganese 0.25 % – 2.0 % 0.50 – 2.0 %
Total Imp. 0.50 % max. 0.50 % max.
Zinc Remainder Remainder
Physical Properties
Condition Size T. S. Mpa EL % Min T. S. Mpa EL % Min
As manufactured All Size 430 min 20 % 460 min 20 %
Cold worked & Stress 10-40 480 min 12 % 520 min 12 %
Relieved 40 above     500 min 15 %
Fabrication Properties
Capacity for being    
Cold Formed Poor Fair
Hot Worked Good Good
Machinability Rating 30 % 30%
Resistance to Corrosion Excellent Excellent
Suitability for Soldering Excellent Fair

NAVAL BRASS RODS - GRADE I & II

IS 291 / 89 NR. EQUIVALENT SPEC. BS 2874 CZ 112, CZ 113,
JIS3250 H C4622 / 41, ASTMBC482 / 8500

Chemical Requirements % Grade I Grade II
Copper 61.0 – 64.0 % 59.0 – 62.0 %
Lead 0.20% max. 0.50 – 1.0 %
Tin 1.0 – 1.50 % 0.50 – 1.0 %
Iron 0.10 max.
Total Imp. 0.20 max. 0.20 % max.
Zinc Remainder Remainder
Physical Properties
Condition Size T. S. kg/mm2 EL % Min T. S. kg/mm2 EL % Min
Half-Hard (HB) Upto 12.5 40 min 18 % 40 min 15%
  12.5 to 50 38.5 min 18 % 40 min 15%
  50 to 100 35 min 18 % 40 min 15%
Fabrication Properties
Capacity for being    
Cold Worked Fair Poor
Hot Worked Excellent Good
Machinability Rating 30% 50%
Forgeability Rating 90% 90%
Silver Alloy Brazing Excellent Good
Soft Soldering Excellent Excellent
Oxyacetylene Welding Good Not Suitable

DEZINCIFICATION RESISTANCE BRASS (DZR)

Standard Specification CW602N
(A) Chemical Requirements % Europe
Copper 61.0 – 63.0 %
Lead 1.70 – 2.8 %
Aluminum 0.05 % max.
Nickel 0.30 % max.
Iron 0.10 % max.
Tin 0.10 % max.
Zinc Remainder
Total Impurities 0.20 % max.
Arsenic 0.02 – 0.15 %
Remarks : Mn <=0.1
(B) Mechanical Properties  
Ultimate Tensile Strength MPa 430 min.
Elongation MPa 200 min.
Hardness HB 110 min.

LEADED COPPER

IS 8328 / 77

Chemical Requirements %
Copper + Ag 99.90 % min
Lead 0.8 – 1.5 %
Physical Properties
Condition T. S. MPa EL % Min
Half-Hard (HB) 260 12 %
Fabrication Properties
Capacity for being Cold Worked Good
Hot Worked Poor
Machiniability Rating 80%
Suitability for Soldering Excellent
Suitability for Brazing Good
Electrical Conductivity 85% IACS

LEADED BRASS FOR SECTION

BS 2874 CZ 130, EN 12167, CW 624 N

Chemical Requirement (%)
Copper 55.50 – 57.50 %
Lead 2.50 – 3.50 %
Aluminum 0.50 % max.
Total Imp. 0.70 % max.
Zinc Remainder
Physical Properties :
Rm – Tensile strength in Mpa 370 min.
Elongation on 5.65 A% 25 min.
Proof strees (0.20%) in Kg/mm2 160 min.
Hardness (HV) 90-120
Fabrication Properties :
Machinability Rating (IS 319-l 100) 100

ARSENICAL COPPER

IS 288 / 81

Chemical Requirements %
Copper + Silver 99.20 % min
Arsenic 0.20 – 16.50 %
Antimony 0.05 % max.
Bismuth 0.002 % max.
Oxygen 0.10 % max
Lead 0.01 % max
Physical Properties
Condition Size T. S. MPa EL % Min
Annealed 10 to 25 215 35%
25 to 50 205 40%
50 & above 195 40%
As Manufactured 10 to 25 255 15%
25 to 50 245 18%
50 & above 235 20%
Fabrication Properties
Capacity for being  
Cold Worked Excellent
Hot Formed Excellent
Suitability for Soldering Good
Suitability for Brazing Good
Suitability for Riveting Excellent

ALUMINUM SILICON BRONZE RODS

IS 10569 / 05 NR. EQUIVALENT SPEC. ASTMBC64200

Chemical Requirements % CuAl7Si2
Copper Remainder
Aluminum 6.3 – 7.60 %
Iron 0.30 % max.
Nickel 0.25 % max.
Manganese 0.10 % max.
Tin 0.20 % max.
Lead 0.05 % max.
Zinc 0.50 % max.
Silicon 1.5 – 2.2 %
Total Imp. Excl. Fe, Ni & Mn 0.50 % max.
Physical Properties
Condition Size T. S. Kg/mm2 EL % Min
Annealed / As Manufactured 6 to 15 620 9%
  15 to 50 575 12%
  50 to 80 515 12%
  80 & above 485 15%
Fabrication Properties
Capacity for being
Cold Worked Not Suitable
Hot Formed Excellent
Machiniability Rating 80%
Suitability for Soldering Excellent
Suitability for Brazing Good

Contact Us for Your Brass Component Needs

we are dedicated to providing high-quality brass components for irrigation and submersible systems. Whether you need detailed product information, pricing, or assistance with selecting the right components for your specific requirements, our team is here to help.

Scroll to Top